项目
限值 / 检出限 / 定量限
单位
出处
最小温度指数
GB/T 23312.1—2009 第15章 · 180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线≥ 180 (180级)15
热冲击温度
GB/T 23312.1—2009 第9章 · 180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线≥ 200 ℃ (180级)℃9
软化击穿
180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线检出要求 (265℃温度下2min内应不击穿)10
耐刮-最小平均刮破力
180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线(导体标称直径2.500mm及以下)≥ 1.45 N (1级,导体标称直径0.250mm)
≥ 1.55 N (1级,导体标称直径0.280mm)
≥ 1.7 N (1级,导体标称直径0.315mm)
≥ 1.8 N (1级,导体标称直径0.355mm)
≥ 1.95 N (1级,导体标称直径0.400mm)
≥ 2.1 N (1级,导体标称直径0.450mm)
≥ 2.25 N (1级,导体标称直径0.500mm)
≥ 2.4 N (1级,导体标称直径0.560mm)
≥ 2.55 N (1级,导体标称直径0.630mm)
≥ 2.75 N (1级,导体标称直径0.710mm)
≥ 2.95 N (1级,导体标称直径0.800mm)
≥ 3.15 N (1级,导体标称直径0.900mm)
≥ 3.4 N (1级,导体标称直径1.000mm)
≥ 3.7 N (1级,导体标称直径1.120mm)
≥ 3.95 N (1级,导体标称直径1.250mm)
≥ 4.25 N (1级,导体标称直径1.400mm)
≥ 4.6 N (1级,导体标称直径1.600mm)
≥ 5.0 N (1级,导体标称直径1.800mm)
≥ 5.3 N (1级,导体标称直径2.000mm)
≥ 5.7 N (1级,导体标称直径2.240mm)
≥ 6.1 N (1级,导体标称直径2.500mm)
≥ 3.15 N (2级,导体标称直径0.400mm)
≥ 3.4 N (2级,导体标称直径0.450mm)
≥ 3.6 N (2级,导体标称直径0.500mm)
≥ 3.85 N (2级,导体标称直径0.560mm)
≥ 4.15 N (2级,导体标称直径0.630mm)
≥ 4.45 N (2级,导体标称直径0.710mm)
≥ 4.75 N (2级,导体标称直径0.800mm)
≥ 5.1 N (2级,导体标称直径0.900mm)
≥ 5.45 N (2级,导体标称直径1.000mm)
≥ 5.8 N (2级,导体标称直径1.120mm)
≥ 6.25 N (2级,导体标称直径1.250mm)
≥ 6.65 N (2级,导体标称直径1.400mm)
≥ 7.15 N (2级,导体标称直径1.600mm)
≥ 7.7 N (2级,导体标称直径1.800mm)
≥ 8.2 N (2级,导体标称直径2.000mm)
≥ 8.75 N (2级,导体标称直径2.240mm)
≥ 9.3 N (2级,导体标称直径2.500mm)N11 表1
耐刮-每次试验中最小刮破力
180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线(导体标称直径2.500mm及以下)≥ 1.25 N (1级,导体标称直径0.250mm)
≥ 1.3 N (1级,导体标称直径0.280mm)
≥ 1.4 N (1级,导体标称直径0.315mm)
≥ 1.55 N (1级,导体标称直径0.355mm)
≥ 1.65 N (1级,导体标称直径0.400mm)
≥ 1.75 N (1级,导体标称直径0.450mm)
≥ 1.9 N (1级,导体标称直径0.500mm)
≥ 2.05 N (1级,导体标称直径0.560mm)
≥ 2.2 N (1级,导体标称直径0.630mm)
≥ 2.35 N (1级,导体标称直径0.710mm)
≥ 2.5 N (1级,导体标称直径0.800mm)
≥ 2.7 N (1级,导体标称直径0.900mm)
≥ 2.9 N (1级,导体标称直径1.000mm)
≥ 3.1 N (1级,导体标称直径1.120mm)
≥ 3.35 N (1级,导体标称直径1.250mm)
≥ 3.6 N (1级,导体标称直径1.400mm)
≥ 3.9 N (1级,导体标称直径1.600mm)
≥ 4.2 N (1级,导体标称直径1.800mm)
≥ 4.5 N (1级,导体标称直径2.000mm)
≥ 4.8 N (1级,导体标称直径2.240mm)
≥ 5.15 N (1级,导体标称直径2.500mm)
≥ 2.65 N (2级,导体标称直径0.400mm)
≥ 2.85 N (2级,导体标称直径0.450mm)
≥ 3.05 N (2级,导体标称直径0.500mm)
≥ 3.25 N (2级,导体标称直径0.560mm)
≥ 3.5 N (2级,导体标称直径0.630mm)
≥ 3.75 N (2级,导体标称直径0.710mm)
≥ 4.05 N (2级,导体标称直径0.800mm)
≥ 4.3 N (2级,导体标称直径0.900mm)
≥ 4.6 N (2级,导体标称直径1.000mm)
≥ 4.9 N (2级,导体标称直径1.120mm)
≥ 5.25 N (2级,导体标称直径1.250mm)
≥ 5.45 N (2级,导体标称直径1.400mm)
≥ 5.85 N (2级,导体标称直径1.600mm)
≥ 6.5 N (2级,导体标称直径1.800mm)
≥ 6.95 N (2级,导体标称直径2.000mm)
≥ 7.4 N (2级,导体标称直径2.240mm)
≥ 7.9 N (2级,导体标称直径2.500mm)N11 表1
最小击穿电压(室温)
180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线(导体标称直径2.500mm及以下)≥ 1900 V (1级,导体标称直径0.250mm)
≥ 2000 V (1级,导体标称直径0.280mm)
≥ 2000 V (1级,导体标称直径0.315mm)
≥ 2100 V (1级,导体标称直径0.355mm)
≥ 2100 V (1级,导体标称直径0.400mm)
≥ 2100 V (1级,导体标称直径0.450mm)
≥ 2200 V (1级,导体标称直径0.500mm)
≥ 2200 V (1级,导体标称直径0.560mm)
≥ 2300 V (1级,导体标称直径0.630mm)
≥ 2300 V (1级,导体标称直径0.710mm)
≥ 2300 V (1级,导体标称直径0.800mm)
≥ 2400 V (1级,导体标称直径0.900mm)
≥ 2400 V (1级,导体标称直径1.000~2.500mm)
≥ 4000 V (2级,导体标称直径0.400mm)
≥ 4000 V (2级,导体标称直径0.450mm)
≥ 4100 V (2级,导体标称直径0.500mm)
≥ 4100 V (2级,导体标称直径0.560mm)
≥ 4300 V (2级,导体标称直径0.630mm)
≥ 4300 V (2级,导体标称直径0.710mm)
≥ 4400 V (2级,导体标称直径0.800mm)
≥ 4500 V (2级,导体标称直径0.900mm)
≥ 4500 V (2级,导体标称直径1.000~2.500mm)V13.1 表2
最小击穿电压(180℃)
180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线(导体标称直径2.500mm及以下)≥ 1400 V (1级,导体标称直径0.250mm)
≥ 1500 V (1级,导体标称直径0.280mm)
≥ 1500 V (1级,导体标称直径0.315mm)
≥ 1600 V (1级,导体标称直径0.355mm)
≥ 1600 V (1级,导体标称直径0.400mm)
≥ 1600 V (1级,导体标称直径0.450mm)
≥ 1700 V (1级,导体标称直径0.500mm)
≥ 1700 V (1级,导体标称直径0.560mm)
≥ 1700 V (1级,导体标称直径0.630mm)
≥ 1700 V (1级,导体标称直径0.710mm)
≥ 1700 V (1级,导体标称直径0.800mm)
≥ 1800 V (1级,导体标称直径0.900mm)
≥ 1800 V (1级,导体标称直径1.000~2.500mm)
≥ 3000 V (2级,导体标称直径0.400mm)
≥ 3000 V (2级,导体标称直径0.450mm)
≥ 3100 V (2级,导体标称直径0.500mm)
≥ 3100 V (2级,导体标称直径0.560mm)
≥ 3200 V (2级,导体标称直径0.630mm)
≥ 3200 V (2级,导体标称直径0.710mm)
≥ 3300 V (2级,导体标称直径0.800mm)
≥ 3400 V (2级,导体标称直径0.900mm)
≥ 3400 V (2级,导体标称直径1.000~2.500mm)V13.1 表2
最小击穿电压(室温)
180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线(导体标称直径2.500mm以上)≥ 1200 V (1级,导体标称直径2.500mm以上)
≥ 2200 V (2级,导体标称直径2.500mm以上)V13.2 表3
最小击穿电压(180℃)
180级聚酯或聚酯亚胺/聚酰胺复合漆包铝圆线(导体标称直径2.500mm以上)≥ 900 V (1级,导体标称直径2.500mm以上)
≥ 1700 V (2级,导体标称直径2.500mm以上)V13.2 表3