项目
限值 / 检出限 / 定量限
单位
出处
球形度S
球形石墨≥ 0.9 (I级)
≥ 0.8 (II级)
≥ 0.6 (III级)4.1 表1
固定碳含量
球形石墨≥ 99.95 % (I级)
≥ 99.9 % (II级)
≥ 99.0 % (III级)%4.1 表1
磁性物质含量
球形石墨≤ 0.1 ppm (I级)
≤ 0.3 ppm (II级)
≤ 0.5 ppm (III级)ppm4.1 表1
铁含量
球形石墨≤ 30 ppm (I级)
≤ 50 ppm (II级)
≤ 70 ppm (III级)ppm4.1 表1
RoHS认证
GB/T 26125 · 球形石墨检出要求 (I级)
检出要求 (II级)
检出要求 (III级)4.1 表1
外观
球形石墨检出要求 (颜色灰黑或钢灰的粉末)5.1
球形度
球形石墨≥ 0.9 (SGI-8-9995-85)
≥ 0.9 (SGI-11-9995-90)
≥ 0.9 (SGI-17-9995-93)
≥ 0.9 (SGI-23-9995-98)
≥ 0.8 (SGII-8-999-80)
≥ 0.8 (SGII-11-999-90)
≥ 0.8 (SGII-17-999-93)
≥ 0.8 (SGII-19-999-90)5.2 表3、表4
粒度分布 D10
球形石墨≥ 5.5 μm (SGI-8-9995-85)
≤ 6.5 μm (SGI-8-9995-85)
≥ 6.0 μm (SGI-11-9995-90)
≤ 7.0 μm (SGI-11-9995-90)
≥ 10.5 μm (SGI-17-9995-93)
≤ 12.0 μm (SGI-17-9995-93)
≥ 13.5 μm (SGI-23-9995-98)
≤ 14.5 μm (SGI-23-9995-98)
≥ 5.0 μm (SGII-8-999-80)
≤ 6.5 μm (SGII-8-999-80)
≥ 6.0 μm (SGII-11-999-90)
≤ 7.0 μm (SGII-11-999-90)
≥ 10.5 μm (SGII-17-999-93)
≤ 12.0 μm (SGII-17-999-93)
≥ 8.5 μm (SGII-19-999-90)
≤ 9.5 μm (SGII-19-999-90)μm5.2 表3、表4
粒度分布 D50
球形石墨≥ 8.0 μm (SGI-8-9995-85)
≤ 9.0 μm (SGI-8-9995-85)
≥ 10.0 μm (SGI-11-9995-90)
≤ 11.0 μm (SGI-11-9995-90)
≥ 16.5 μm (SGI-17-9995-93)
≤ 18.5 μm (SGI-17-9995-93)
≥ 20.5 μm (SGI-23-9995-98)
≤ 22.5 μm (SGI-23-9995-98)
≥ 8.0 μm (SGII-8-999-80)
≤ 10.0 μm (SGII-8-999-80)
≥ 10.0 μm (SGII-11-999-90)
≤ 11.0 μm (SGII-11-999-90)
≥ 16.5 μm (SGII-17-999-93)
≤ 18.5 μm (SGII-17-999-93)
≥ 19.0 μm (SGII-19-999-90)
≤ 20.0 μm (SGII-19-999-90)μm5.2 表3、表4
粒度分布 D90
球形石墨≥ 12.0 μm (SGI-8-9995-85)
≤ 14.0 μm (SGI-8-9995-85)
≥ 16.0 μm (SGI-11-9995-90)
≤ 19.0 μm (SGI-11-9995-90)
≥ 24.5 μm (SGI-17-9995-93)
≤ 28.5 μm (SGI-17-9995-93)
≥ 32.0 μm (SGI-23-9995-98)
≤ 34.0 μm (SGI-23-9995-98)
≥ 12.0 μm (SGII-8-999-80)
≤ 15.0 μm (SGII-8-999-80)
≥ 16.0 μm (SGII-11-999-90)
≤ 19.0 μm (SGII-11-999-90)
≥ 24.5 μm (SGII-17-999-93)
≤ 28.5 μm (SGII-17-999-93)
≥ 37.0 μm (SGII-19-999-90)
≤ 38.5 μm (SGII-19-999-90)μm5.2 表3、表4
粒度分布 Dmax
球形石墨≤ 23.0 μm (SGI-8-9995-85)
≤ 30.0 μm (SGI-11-9995-90)
≤ 45.0 μm (SGI-17-9995-93)
≤ 60.0 μm (SGI-23-9995-98)
≤ 23.0 μm (SGII-8-999-80)
≤ 30.0 μm (SGII-11-999-90)
≤ 45.0 μm (SGII-17-999-93)
≤ 60.0 μm (SGII-19-999-90)μm5.2 表3、表4
固定碳
球形石墨≥ 99.95 % (SGI-8-9995-85)
≥ 99.95 % (SGI-11-9995-90)
≥ 99.95 % (SGI-17-9995-93)
≥ 99.95 % (SGI-23-9995-98)
≥ 99.9 % (SGII-8-999-80)
≥ 99.9 % (SGII-11-999-90)
≥ 99.9 % (SGII-17-999-93)
≥ 99.9 % (SGII-19-999-90)%5.2 表3、表4
水分
球形石墨≤ 0.2 % (SGI-8-9995-85)
≤ 0.2 % (SGI-11-9995-90)
≤ 0.1 % (SGI-17-9995-93)
≤ 0.1 % (SGI-23-9995-98)
≤ 0.2 % (SGII-8-999-80)
≤ 0.2 % (SGII-11-999-90)
≤ 0.2 % (SGII-17-999-93)
≤ 0.2 % (SGII-19-999-90)%5.2 表3、表4
pH值
球形石墨≥ 4.5 (SGI-8-9995-85)
≤ 6 (SGI-8-9995-85)
≥ 4.5 (SGI-11-9995-90)
≤ 6 (SGI-11-9995-90)
≥ 4.5 (SGI-17-9995-93)
≤ 6 (SGI-17-9995-93)
≥ 4.5 (SGI-23-9995-98)
≤ 6 (SGI-23-9995-98)
≥ 4.5 (SGII-8-999-80)
≤ 5.5 (SGII-8-999-80)
≥ 4.5 (SGII-11-999-90)
≤ 5.5 (SGII-11-999-90)
≥ 4.5 (SGII-17-999-93)
≤ 5.5 (SGII-17-999-93)
≥ 4.5 (SGII-19-999-90)
≤ 5.5 (SGII-19-999-90)5.2 表3、表4
振实密度
球形石墨≥ 0.85 g/cm3 (SGI-8-9995-85)
≥ 0.9 g/cm3 (SGI-11-9995-90)
≥ 0.93 g/cm3 (SGI-17-9995-93)
≥ 0.98 g/cm3 (SGI-23-9995-98)
≥ 0.8 g/cm3 (SGII-8-999-80)
≥ 0.9 g/cm3 (SGII-11-999-90)
≥ 0.93 g/cm3 (SGII-17-999-93)
≥ 0.9 g/cm3 (SGII-19-999-90)g/cm35.2 表3、表4
比表面积
球形石墨≥ 9.5 m2/g (SGI-8-9995-85)
≤ 10.5 m2/g (SGI-8-9995-85)
≥ 7.0 m2/g (SGI-11-9995-90)
≤ 8.5 m2/g (SGI-11-9995-90)
≥ 5.0 m2/g (SGI-17-9995-93)
≤ 6.5 m2/g (SGI-17-9995-93)
≥ 4.5 m2/g (SGI-23-9995-98)
≤ 6.0 m2/g (SGI-23-9995-98)
≥ 9.5 m2/g (SGII-8-999-80)
≤ 11.0 m2/g (SGII-8-999-80)
≥ 7.0 m2/g (SGII-11-999-90)
≤ 9.0 m2/g (SGII-11-999-90)
≥ 5.5 m2/g (SGII-17-999-93)
≤ 7.0 m2/g (SGII-17-999-93)
≥ 5.0 m2/g (SGII-19-999-90)
≤ 6.5 m2/g (SGII-19-999-90)m2/g5.2 表3、表4
铁
球形石墨≤ 30.0 ppm (SGI-8-9995-85)
≤ 30.0 ppm (SGI-11-9995-90)
≤ 30.0 ppm (SGI-17-9995-93)
≤ 30.0 ppm (SGI-23-9995-98)
≤ 50.0 ppm (SGII-8-999-80)
≤ 50.0 ppm (SGII-11-999-90)
≤ 50.0 ppm (SGII-17-999-93)
≤ 50.0 ppm (SGII-19-999-90)ppm5.2 表3、表4
钠
球形石墨≤ 10.0 ppm (SGI-8-9995-85)
≤ 10.0 ppm (SGI-11-9995-90)
≤ 10.0 ppm (SGI-17-9995-93)
≤ 10.0 ppm (SGI-23-9995-98)
≤ 20.0 ppm (SGII-8-999-80)
≤ 20.0 ppm (SGII-11-999-90)
≤ 20.0 ppm (SGII-17-999-93)
≤ 20.0 ppm (SGII-19-999-90)ppm5.2 表3、表4
铬
球形石墨≤ 10.0 ppm (SGI-8-9995-85)
≤ 10.0 ppm (SGI-11-9995-90)
≤ 10.0 ppm (SGI-17-9995-93)
≤ 10.0 ppm (SGI-23-9995-98)
≤ 20.0 ppm (SGII-8-999-80)
≤ 20.0 ppm (SGII-11-999-90)
≤ 20.0 ppm (SGII-17-999-93)
≤ 20.0 ppm (SGII-19-999-90)ppm5.2 表3、表4
铜
球形石墨≤ 10.0 ppm (SGI-8-9995-85)
≤ 10.0 ppm (SGI-11-9995-90)
≤ 10.0 ppm (SGI-17-9995-93)
≤ 10.0 ppm (SGI-23-9995-98)
≤ 20.0 ppm (SGII-8-999-80)
≤ 20.0 ppm (SGII-11-999-90)
≤ 20.0 ppm (SGII-17-999-93)
≤ 20.0 ppm (SGII-19-999-90)ppm5.2 表3、表4
镍
球形石墨≤ 10.0 ppm (SGI-8-9995-85)
≤ 10.0 ppm (SGI-11-9995-90)
≤ 10.0 ppm (SGI-17-9995-93)
≤ 10.0 ppm (SGI-23-9995-98)
≤ 20.0 ppm (SGII-8-999-80)
≤ 20.0 ppm (SGII-11-999-90)
≤ 20.0 ppm (SGII-17-999-93)
≤ 20.0 ppm (SGII-19-999-90)ppm5.2 表3、表4
球形度
球形石墨≥ 0.6 (SGIII-8-99-75)
≥ 0.6 (SGIII-11-99-90)
≥ 0.6 (SGIII-17-99-92)
≥ 0.6 (SGIII-19-99-95)表5
D10
球形石墨≥ 4.0 μm (SGIII-8-99-75)
≤ 5.0 μm (SGIII-8-99-75)
≥ 5.5 μm (SGIII-11-99-90)
≤ 7.5 μm (SGIII-11-99-90)
≥ 10.0 μm (SGIII-17-99-92)
≤ 12.0 μm (SGIII-17-99-92)
≥ 8.5 μm (SGIII-19-99-95)
≤ 10.0 μm (SGIII-19-99-95)μm表5
D50
球形石墨≥ 7.5 μm (SGIII-8-99-75)
≤ 8.5 μm (SGIII-8-99-75)
≥ 10.0 μm (SGIII-11-99-90)
≤ 11.5 μm (SGIII-11-99-90)
≥ 16.5 μm (SGIII-17-99-92)
≤ 18.5 μm (SGIII-17-99-92)
≥ 19.0 μm (SGIII-19-99-95)
≤ 20.0 μm (SGIII-19-99-95)μm表5
D90
球形石墨≥ 14.0 μm (SGIII-8-99-75)
≤ 16.0 μm (SGIII-8-99-75)
≥ 16.0 μm (SGIII-11-99-90)
≤ 21.0 μm (SGIII-11-99-90)
≥ 25.0 μm (SGIII-17-99-92)
≤ 29.0 μm (SGIII-17-99-92)
≥ 37.0 μm (SGIII-19-99-95)
≤ 39.0 μm (SGIII-19-99-95)μm表5
Dmax
球形石墨≤ 30 μm (SGIII-8-99-75)
≤ 45.0 μm (SGIII-11-99-90)
≤ 60.0 μm (SGIII-17-99-92)
≤ 60.0 μm (SGIII-19-99-95)μm表5
固定碳
球形石墨≥ 99.0 % (SGIII-8-99-75)
≥ 99.0 % (SGIII-11-99-90)
≥ 99.0 % (SGIII-17-99-92)
≥ 99.0 % (SGIII-19-99-95)%表5
水分
球形石墨≤ 0.5 % (SGIII-8-99-75)
≤ 0.3 % (SGIII-11-99-90)
≤ 0.3 % (SGIII-17-99-92)
≤ 0.3 % (SGIII-19-99-95)%表5
pH值
球形石墨≥ 4 (SGIII-8-99-75)
≤ 5.5 (SGIII-8-99-75)
≥ 4 (SGIII-11-99-90)
≤ 5.5 (SGIII-11-99-90)
≥ 4 (SGIII-17-99-92)
≤ 5.5 (SGIII-17-99-92)
≥ 4 (SGIII-19-99-95)
≤ 5.5 (SGIII-19-99-95)表5
振实密度
球形石墨≥ 0.75 g/cm3 (SGIII-8-99-75)
≥ 0.9 g/cm3 (SGIII-11-99-90)
≥ 0.92 g/cm3 (SGIII-17-99-92)
≥ 0.95 g/cm3 (SGIII-19-99-95)g/cm3表5
比表面积
球形石墨≥ 9.0 m2/g (SGIII-8-99-75)
≤ 11.5 m2/g (SGIII-8-99-75)
≥ 8.0 m2/g (SGIII-11-99-90)
≤ 10.0 m2/g (SGIII-11-99-90)
≥ 5.5 m2/g (SGIII-17-99-92)
≤ 7.5 m2/g (SGIII-17-99-92)
≥ 5.0 m2/g (SGIII-19-99-95)
≤ 6.5 m2/g (SGIII-19-99-95)m2/g表5
铁
球形石墨≤ 70.0 ppm (SGIII-8-99-75)
≤ 70.0 ppm (SGIII-11-99-90)
≤ 70.0 ppm (SGIII-17-99-92)
≤ 70.0 ppm (SGIII-19-99-95)ppm表5
钠
球形石墨≤ 20.0 ppm (SGIII-8-99-75)
≤ 20.0 ppm (SGIII-11-99-90)
≤ 20.0 ppm (SGIII-17-99-92)
≤ 20.0 ppm (SGIII-19-99-95)ppm表5
铬
球形石墨≤ 20.0 ppm (SGIII-8-99-75)
≤ 20.0 ppm (SGIII-11-99-90)
≤ 20.0 ppm (SGIII-17-99-92)
≤ 20.0 ppm (SGIII-19-99-95)ppm表5
铜
球形石墨≤ 20.0 ppm (SGIII-8-99-75)
≤ 20.0 ppm (SGIII-11-99-90)
≤ 20.0 ppm (SGIII-17-99-92)
≤ 20.0 ppm (SGIII-19-99-95)ppm表5
镍
球形石墨≤ 20.0 ppm (SGIII-8-99-75)
≤ 20.0 ppm (SGIII-11-99-90)
≤ 20.0 ppm (SGIII-17-99-92)
≤ 20.0 ppm (SGIII-19-99-95)ppm表5
铝
球形石墨≤ 20.0 ppm (SGIII-8-99-75)
≤ 20.0 ppm (SGIII-11-99-90)
≤ 20.0 ppm (SGIII-17-99-92)
≤ 20.0 ppm (SGIII-19-99-95)ppm表5
钼
球形石墨≤ 20.0 ppm (SGIII-8-99-75)
≤ 20.0 ppm (SGIII-11-99-90)
≤ 20.0 ppm (SGIII-17-99-92)
≤ 20.0 ppm (SGIII-19-99-95)ppm表5
锌
球形石墨≤ 20.0 ppm (SGIII-8-99-75)
≤ 20.0 ppm (SGIII-11-99-90)
≤ 20.0 ppm (SGIII-17-99-92)
≤ 20.0 ppm (SGIII-19-99-95)ppm表5
钴
球形石墨≤ 20.0 ppm (SGIII-8-99-75)
≤ 20.0 ppm (SGIII-11-99-90)
≤ 20.0 ppm (SGIII-17-99-92)
≤ 20.0 ppm (SGIII-19-99-95)ppm表5
硅
球形石墨≤ 500 ppm (SGIII-8-99-75)
≤ 500 ppm (SGIII-11-99-90)
≤ 500 ppm (SGIII-17-99-92)
≤ 500 ppm (SGIII-19-99-95)ppm表5
磁性物质(铁+铬+镍+锌+钴)
球形石墨≤ 0.5 ppm (SGIII-8-99-75)
≤ 0.5 ppm (SGIII-11-99-90)
≤ 0.5 ppm (SGIII-17-99-92)
≤ 0.5 ppm (SGIII-19-99-95)ppm表5
硫含量
球形石墨≤ 200 ppm (SGIII-8-99-75)
≤ 200 ppm (SGIII-11-99-90)
≤ 200 ppm (SGIII-17-99-92)
≤ 200 ppm (SGIII-19-99-95)ppm表5
镉及其化合物
球形石墨≤ 20 ppm (SGIII-8-99-75)
≤ 20 ppm (SGIII-11-99-90)
≤ 20 ppm (SGIII-17-99-92)
≤ 20 ppm (SGIII-19-99-95)ppm表5
铅及其化合物
球形石墨≤ 20 ppm (SGIII-8-99-75)
≤ 20 ppm (SGIII-11-99-90)
≤ 20 ppm (SGIII-17-99-92)
≤ 20 ppm (SGIII-19-99-95)ppm表5
汞及其化合物
球形石墨≤ 20 ppm (SGIII-8-99-75)
≤ 20 ppm (SGIII-11-99-90)
≤ 20 ppm (SGIII-17-99-92)
≤ 20 ppm (SGIII-19-99-95)ppm表5
六价铬及其化合物
球形石墨≤ 20 ppm (SGIII-8-99-75)
≤ 20 ppm (SGIII-11-99-90)
≤ 20 ppm (SGIII-17-99-92)
≤ 20 ppm (SGIII-19-99-95)ppm表5
F-
球形石墨≤ 20 ppm (SGIII-8-99-75)
≤ 20 ppm (SGIII-11-99-90)
≤ 20 ppm (SGIII-17-99-92)
≤ 20 ppm (SGIII-19-99-95)ppm表5
Cl-
球形石墨≤ 100 ppm (SGIII-8-99-75)
≤ 100 ppm (SGIII-11-99-90)
≤ 100 ppm (SGIII-17-99-92)
≤ 100 ppm (SGIII-19-99-95)ppm表5
Br-
球形石墨≤ 100 ppm (SGIII-8-99-75)
≤ 100 ppm (SGIII-11-99-90)
≤ 100 ppm (SGIII-17-99-92)
≤ 100 ppm (SGIII-19-99-95)ppm表5
NO3-
球形石墨≤ 100 ppm (SGIII-8-99-75)
≤ 100 ppm (SGIII-11-99-90)
≤ 100 ppm (SGIII-17-99-92)
≤ 100 ppm (SGIII-19-99-95)ppm表5
SO4^2-
球形石墨≤ 100 ppm (SGIII-8-99-75)
≤ 100 ppm (SGIII-11-99-90)
≤ 100 ppm (SGIII-17-99-92)
≤ 100 ppm (SGIII-19-99-95)ppm表5
外观—6.1
粒度分布
GB/T 24533—2019 附录A—6.2
水分
GB/T 24533—2019 附录B—6.3
pH值
GB/T 24533—2019 附录C—6.4
固定碳含量
GB/T 3521—6.5
比表面积
GB/T 19587—6.6
球形度
附录A—6.7
振实密度
GB/T 24533—2019 附录M—6.8
磁性物质
GB/T 24533—2019 附录K—6.9
微量金属元素
附录B—6.10
硫含量
GB/T 24533—2019 附录J—6.11
F⁻、Cl⁻、Br⁻、SO₄²⁻、NO₃⁻
GB/T 24533—2019 附录I—6.12
限用物质含量
GB/T 26125—6.13